Skip to main content

Table 5 The parameters of power-law model and the hysteresis loop area values obtained from shear loop test of the different ratios of LPSG-XG blendsa,b

From: Rheological properties of binary mixtures of Lepidium perfoliatum seed gum and xanthan gum

LPSG-XG (%)

Forward

Backward

Hysteresis loop area (%)

kp (Pa.sn)

np

R2

kʹp (Pa.sn)

n′p

R2

LPSG0-XG100

22.54 ± 1.86a

0.08 ± 0.01c

0.91

3.51 ± 0.22a

0.38 ± 0.02c

0.98

20.86

LPSG25-XG75

2.40 ± 0.08b

0.33 ± 0.07b

0.99

0.81 ± 0.04b

0.50 ± 0.05b

0.99

13.74

LPSG50-XG50

0.91 ± 0.05c

0.44 ± 0.03a

0.99

0.70 ± 0.06c

0.48 ± 0.03b

0.99

4.29

LPSG75-XG25

0.47 ± 0.02d

0.40 ± 0.06a

0.98

0.10 ± 0.02e

0.64 ± 0.03a

0.99

19.35

LPSG100-XG0

0.49 ± 0.04d

0.41 ± 0.04a

0.95

0.17 ± 0.03d

0.60 ± 0.05a

0.99

0.88

  1. aValues in columns with different letters are significantly different (P ≤ 0.05)
  2. bLPSG Lepidium perfoliatum seed gum, XG xanthan gum